Specimen Information
Name: BRI No. 3 (Japan), ws26bs
Type: Spiral
Comments: square cross-section
Reference: Kenchiku Kenkyu Siryo No. 21, "Aseismic Analysis of Building Structural Members: a List of Experimental Results on Deformation Ability of Reinforced Concrete Columns Under Large Deflection (No.3)," Building Research Institute, Ministry of Construction, Ja
Material Properties
Concrete Strength:31.6 (MPa)
Transverse Steel:Yield Stress: 386.5 (MPa)
Longitudinal Steel:Yield Stress: 382 (MPa) Strength: 0 (MPa)
Geometry
Diameter: 250 (mm) Cross-Section: Square
Length: L-Inflection: 500 (mm) L-Measured: 500 (mm)
Test Configuration:Double Cantilever
Loading
Axial Load:161 (kN)
P-D:Shear provided
L-Bottom:0
Longitudinal Reinforcement
Diameter:12.7 (mm)
Number of Bars:8
Reinforcement Ratio:0.0162
Transverse Reinforcement
Diameter Spiral:3.9 (mm)
Hoop Spacing, Sv:37 (mm)
Cover to Center of Hoop Bar:37 (mm)
Reinforcement Ratio:0.75
Non-Dimensional Properties
Span-to-Depth Ratio:2
Axial Load Ratio:0.082
Test Results
Failure Type:Flexure-Shear
Damage Observation:Concrete Crushing: 0 (mm)
Significant Concrete Spalling: 0 (mm)
Long Bar Buckling: 0 (mm)
Long Bar Fracture: 0 (mm)
Spiral Fracture: 0 (mm)
Loss of Axial Load Capacity: 0 (mm)
Resources:Force-Displacement Hysteresis (graph)
Force Displacement Data (data)
Record Information
Version:1 (April 8, 2003)
The Structural Performance Database is a project of the Pacific Earthquake Engineering Research Center, funded by the National Science Foundation. Contact Marc Eberhard at the University of Washington with questions or comments. Report technical problems to the server administrator. Copyright 2003.