Specimen Information
Name: Munro et al. 1976, No. 1
Type: Spiral
Comments: Specimen had pier cap,not tested to failure
Reference: Munro, I.R.M.; Park, R.; and Priestley, M.J.N., Seismic Behaviour of Reinforced Concrete Bridge Piers, Report 76-9, Department of Civil Engineering, University of Canterbury, Christchurch, New Zealand, February 1976, 106 pages.
Material Properties
Concrete Strength:40 (MPa)
Transverse Steel:Yield Stress: 389 (MPa)
Longitudinal Steel:Yield Stress: 305 (MPa) Strength: 411 (MPa)
Geometry
Diameter: 500 (mm) Cross-Section: Octagonal
Length: L-Inflection: 2,730 (mm) L-Measured: 2,730 (mm)
Test Configuration:Cantilever with Hammer Head
Loading
Axial Load:26.4 (kN)
P-D:Feff provided
L-Bottom:0
Longitudinal Reinforcement
Diameter:18.4 (mm)
Number of Bars:20
Reinforcement Ratio:0.0257
Transverse Reinforcement
Diameter Spiral:8 (mm)
Hoop Spacing, Sv:34 (mm)
Cover to Center of Hoop Bar:20.2 (mm)
Reinforcement Ratio:1.26
Non-Dimensional Properties
Span-to-Depth Ratio:5.46
Axial Load Ratio:0.003
Test Results
Failure Type:Flexure
Damage Observation:Concrete Crushing: 38 (mm)
Significant Concrete Spalling: 76 (mm)
Long Bar Buckling: 0 (mm)
Long Bar Fracture: 0 (mm)
Spiral Fracture: 0 (mm)
Loss of Axial Load Capacity: 0 (mm)
Resources:Force-Displacement Hysteresis (graph)